Electrode e Tlase ea Haedrojene ea AWS E8015-G Electrode e Tlase ea Tšepe e nang le Alloy e Tlase

Tlhaloso e Khutšoanyane:

J557 (AWS E8015-G) ke electrode ea tšepe e nang le motsoako o tlase e nang le hydrogen sodium e tlase. Sebelisa DCEP (electrode ea hona joale e tobileng e ntle), 'me e ka kopanngoa libakeng tsohle.


Qaqiso ea Sehlahisoa

Li-tag tsa Sehlahisoa

Electrode ea ho Welding ea Tšepe e Tlase ea Motsoako o Tlase

J557                                             

GB/T E5515-G

AWS E8015-G

Tlhaloso: J557 ke electrode ea tšepe e nang le motsoako o tlase e nang le hydrogen sodium e tlase. Sebelisa DCEP (electrode ea hona joale e tobileng e ntle), 'me e ka kopanngoa maemong 'ohle.

Tšebeliso: E sebelisetsoa ho tjheseletsa tšepe ea khabone e mahareng le meaho ea tšepe e nang le motsoako o tlase joalo ka Q390.

 

Sebopeho sa lik'hemik'hale sa tšepe e welded (%):

C

Mn

Si

S

P

≤0.12

≥1.00

0.30 ~ 0.70

≤0.035

≤0.035

 

Litšobotsi tsa mechini tsa tšepe e welded:

Ntho ea teko

Matla a tšepe

Mpa

Matla a tlhahiso

Mpa

Ho lelefatsa

%

Boleng ba tšusumetso (J)

-20℃

-30℃

E tiiselitsoe

≥540

≥440

≥17

—

≥27

 

Tekanyo ea haedrojene e hasaneng ea tšepe e bolokiloeng: ≤6.0mL/100g (mokhoa oa glycerin)

Tlhahlobo ea X-ray: Kereiti ea I

 

Khoeli e khothaletsoang:

(mm)

Bophara ba molamu

2.5

3.2

4.0

5.0

(A)

ho tjheseletsa hona joale

60 ~ 90

80 ~ 110

130 ~ 170

160 ~ 200

 

Tsebiso:

1. Electrode e lokela ho besoa hora e le 'ngoe mochesong o ka bang 350℃ pele ho ts'ebetso ea ho tjheseletsa;

2. Ho bohlokoa ho hlwekisa mafome, sekala sa oli, metsi le litšila likarolong tsa ho tjheseletsa pele ho tjheseletsa;

3. Sebelisa ts'ebetso e khutšoanyane ea arc ha u tjheseletsa. Tsela e moqotetsane ea ho tjheseletsa e loketse.

 

Wenzhou Tianyu Electronic Co., Ltd. e thehiloe ka selemo sa 2000. Re ntse re etsa tlhahiso eaelektrode ea ho tjheseletsas, lithupa tsa ho tjheseletsa, le lintho tse sebelisoang ho tjheseletsa ka lilemo tse fetang 20.

Lihlahisoa tsa rona tse ka sehloohong li kenyelletsa tšepe e sa hloekangelektrode ea ho tjheseletsas, li-electrode tsa ho tjheseletsa tšepe ea khabone,li-electrode tsa ho tjheseletsa tse nang le motsoako o tlase, li-electrode tsa ho tjheseletsa holim'a metsi, li-electrode tsa ho tjheseletsa ka alloy ea nickel & cobalt, lithapo tsa ho tjheseletsa tsa tšepe e bobebe le alloy e tlase, lithapo tsa ho tjheseletsa tsa tšepe e sa ruseng, lithapo tse sirelelitsoeng ka khase, lithapo tsa ho tjheseletsa tsa aluminium, ho tjheseletsa ka arc e ka tlas'a metsi. lithapo, lithapo tsa ho tjheseletsa ka alloy ea nickel & cobalt, lithapo tsa ho tjheseletsa tsa koporo, lithapo tsa ho tjheseletsa tsa TIG & MIG, li-electrode tsa tungsten, li-electrode tse sehang khabone, le lisebelisoa tse ling tsa ho tjheseletsa le tse sebelisoang.

 


  • E fetileng:
  • E 'ngoe: