Terata ea ho tjheseletsa ea motsoako oa nikeli ea ERNiCrMo-3 Tig

Tlhaloso e Khutšoanyane:

ERNiCrMo-3 ke terata e nang le motsoako o phahameng oa nickel e etselitsoeng ho tjheseletsa le ho koahela metsoako e thehiloeng ho nickel e kang 625 kapa thepa e tšoanang.


Qaqiso ea Sehlahisoa

Li-tag tsa Sehlahisoa

Motsoako oa nikeleTerata ea ho tjheseletsaTerata ea TigERNiCrMo-3

 

Likarolo le Litšebeliso

Holimonikeliterata ea motsoako e entsoeng bakeng sa ho tjheseletsa le ho koahelanikelimetsoako e thehiloeng ho yona e kang 625 kapa thepa e tshwanang.

E huloa ka tsela e ikhethang haholo ho fumana li-weld tse hloekileng le tsa boleng bo holimo tse nang le moalo o khanyang le ho se sebetse hantle haholo.

Tšepe e welded e na le thepa e ntle haholo ea mechini mochesong o phahameng le o tlase.

Ho hanyetsa hantle ho ts'enyeho ea pitting le khatello ea maikutlo.

Mocheso o khothaletsoang oa ho sebetsa o tloha ho cryogenic ho isa ho 540°C.

Hangata e sebelisoa indastering ea ts'ebetso ea lik'hemik'hale, boenjiniere ba likepe, likarolo tsa reactor ea nyutlelie, lifofane le ka har'a lisebelisoa tsa taolo ea tšilafalo jj.

Lisebelisoa tse Tloaelehileng tsa Motheo

Inconel 601, Incoloy 800, Motsoako o kopantsoeng 625, Motsoako o kopantsoeng 825, Motsoako o kopantsoeng 926*
* Lethathamo le hlalosang, eseng le felletseng

 

Maemo
EN ISO 18274 - Ni 6625 - NiCr22Mo9Nb
AWS A5.14 – ER NiCrMo-3

 

Sebopeho sa Lik'hemik'hale %

C%

Mn%

Fe%

P%

S%

Si%

Cu%

boholo

boholo

boholo

boholo

boholo

boholo

boholo

0.10

0.50

0.50

0.015

0.015

0.50

0.50

Ni%

Co%

Al%

Ti%

Cr%

Nb+Ta%

Mo%

60.00

boholo

boholo

boholo

20.00

3.15

8.00

motsotso

1.0

0.40

0.40

23.00

4.15

10.00

 

Matlotlo a Mekaniki
Matla a tšepe ≥760 MPa  
Matla a Tekanyo ≥415 MPa  
Ho lelefatsa ≥35%  
Matla a Tšusumetso ≥100 J  

Thepa ea mechini ke ea khakanyo 'me e ka fapana ho latela mocheso, khase e sireletsang, liparamente tsa ho tjheseletsa le lintlha tse ling.

 

Likhase tse Sireletsang

TS EN ISO 14175 TIG: I1 (Argon)

 

Maemo a ho tjheseletsa

TS EN ISO 6947 PA, PB, PC, PD, PE, PF, PG

 

Lintlha tsa ho paka
Bophara Bolelele Boima ba 'mele  
1.60 mm

2.40 mm

3.20 mm

1000 mm

1000 mm

1000 mm

5 kg

5 kg

5 kg

 

 

Boikarabello: Le hoja ho entsoe boiteko bohle bo utloahalang ho netefatsa ho nepahala ha tlhahisoleseling e ka har'a eona, tlhahisoleseling ena e ka fetoha ntle le tsebiso 'me e ka nkoa e loketse feela bakeng sa tataiso e akaretsang.

 


  • E fetileng: