Li-electrode tsa ho tjheseletsa tsa tšepe ea k'habone tsa AWS E7014 J501Fe Liropo tsa ho tjheseletsa tsa tšepe e bonolo

Tlhaloso e Khutšoanyane:

J501Fe (AWS E7014) ke phofo ea tšepe le elektrode e koahetsoeng ka mofuta oa titanium oxide.


Qaqiso ea Sehlahisoa

Li-tag tsa Sehlahisoa

Electrode ea ho tjheseletsa ea Tšepe ea Khabone

J501Fe

GB/T E5014

AWS A5.1 E7014

Tlhaloso: J501Fe ke electrode e koahetsoeng ka phofo ea tšepe le mofuta oa titanium oxide. E ka sebelisoa bakeng sa ho tjheseletsa libaka tsohle ka AC le DC, katleho ea ho boloka ke hoo e ka bang 110%.

Kopo: Bakeng sa meaho ea tšepe ea carbon le tšepe e nang le motsoako o tlase, joalo ka Q345 le likepe tse ling, likoloi le meaho ea mechini ea ho tjheseletsa.

Sebopeho sa lik'hemik'hale sa tšepe e welded (%):

C

Mn

Si

S

P

≤0.12

≤1.25

≤0.60

≤0.035

≤0.035

 

Litšobotsi tsa mechini tsa tšepe e welded:

Ntho ea teko

Matla a tšepe

Mpa

Matla a tlhahiso

Mpa

Ho lelefatsa

%

Boleng ba tšusumetso (J)

0℃

E tiiselitsoe

≥490

≥400

≥17

≥27

E lekiloe

520 ~ 580

≥410

17 ~ 26

50 ~ 100

 

Tlhahlobo ea X-ray: Kereiti ea II

Khoeli e khothaletsoang:

Bophara ba molamu

(mm)

2.0

2.5

3.2

4.0

5.0

5.8

Hona joale ho tjheseletsa

(A)

40 ~ 70

70 ~ 90

90 ~ 130

160 ~ 210

210 ~ 250

260 ~ 310

 

Wenzhou Tianyu Electronic Co., Ltd. e thehiloe ka selemo sa 2000. Re 'nile ra kopanela tlhahisong ea li-electrode tsa ho tjheseletsa, lithupa tsa ho tjheseletsa le lisebelisoa tse sebelisoang tsa ho tjheseletsa ka lilemo tse fetang 20.

Lihlahisoa tsa rona tse ka sehloohong li kenyelletsa li-electrode tsa tšepe e sa hloekang, li-electrode tsa tšepe ea khabone, li-electrode tsa ho tjheseletsa tse nang le alloy e tlase, li-electrode tsa ho tjheseletsa tse holim'a metsi, li-electrode tsa ho tjheseletsa tse nang le alloy ea nickel & cobalt, lithapo tsa ho tjheseletsa tse nang le alloy e bobebe le e nang le alloy e tlase, lithapo tsa ho tjheseletsa tse nang le alloy e sirelelitsoeng ke khase, lithapo tsa ho tjheseletsa tsa aluminium, ho tjheseletsa ka har'a arc e ka tlas'a metsi. lithapo, lithapo tsa ho tjheseletsa tse nang le alloy ea nickel & cobalt, lithapo tsa ho tjheseletsa tsa koporo, lithapo tsa ho tjheseletsa tsa TIG & MIG, li-electrode tsa tungsten, li-electrode tse sehang khabone, le lisebelisoa tse ling tsa ho tjheseletsa le tse sebelisoang.

 

 


  • E fetileng:
  • E 'ngoe: